骨瓷釉(you)系列(lie)先容

Bone china glaze series introduction

 

品名(ming) 编号 烧成温度 体收(shou)缩 利用申明
Type Item No Tempreture COE Application
新磁器 fine china DP-1 1120-1140℃ 152

The operation steps as follows
1.Add more than 30% water into the glaze lump, mix completely and leave for over 2hours.
2.Loading the glaze into mill machine grind 2 hours.
3.removing iron and filtration , sieving through 200 mesh.
4.adjust density to 60-65 degree.
5. keep the high gap at the 1-1.5 meters from the glaze tub to spray gun.
6.install a pressure regulator in front of spray gun, and adjust the pressure at the 0.8-1.2mm.
7.after glaze firing temperature reach to setting degree. Keep heat on 20-25 minutes.
8.after heat preservation open the kiln door by a third.
9.quickly cool itself. The glaze will achieve to good effect.

 

操纵步骤以下:
1.将30%以上的水插手釉块内,均匀浸泡2小时以上
2.将釉料装入球磨机内磨2小时.
3.除铁和过滤,经由过程200目筛。
4.调剂浓度为60-65度.
5.釉桶与喷枪高位差异为1-1.5米。
6.在喷枪前装置压力调理器,调理压力为2Mpa,喷釉厚度为0.8-1.2mm.
7.釉烧后温度到达设定度,保温20-25分钟。
8.保温后,将窑门翻开三分之一。
9.即速天然降温,釉面到达更佳结果

新骨瓷 New bone BO-3 1120-1140℃ 208
老磁器 old china DP-1 1120-1140℃ 152
BO-3 1120-1140℃ 208

 

骨瓷釉